Arte SheetsLearn. Try. Understand.

Metallurgical Quench Hardenability, ASTM A255 Jominy/Grossmann DI & Alloy Steels

ASTM A255 Grossmann Steel Hardenability (DI) Formula

Calculate Manganese Multiplying Factor f_Mn, Combined Alloy Hardenability Product (Mn*Cr*Mo*Ni), Ideal Critical Bar Diameter DI in Millimeters, and DI in Inches.

Carbon sets MAXIMUM martensite hardness—Cr, Mo, and Mn MULTIPLY how deep martensite hardens into thick shaft cores

Beginner heat-treaters confuse Hardness (surface HRC controlled almost solely by %C) with Hardenability (how thick a round bar transforms to >= 50% martensite at its center before slow cooling forms soft pearlite/bainite). Marcus Grossmann (1942, standardized in ASTM A255) proved that alloying elements retard diffusive pearlite nucleation MULTIPLICATIVELY rather than additively. Starting from Base Carbon-plus-Grain-Size Diameter D_I0 (mm, e.g. 5.4 mm for 0.40% C at ASTM Grain Size #7), multiplying ASTM A255 linear alloy factors f_Mn = 1 + 3.333 * %Mn (<= 1.2%), f_Cr = 1 + 2.160 * %Cr (<= 1.5%), f_Mo = 1 + 3.000 * %Mo (<= 0.4%), and f_Ni = 1 + 0.363 * %Ni (<= 1.5%) yields **Ideal Critical Diameter D_I = D_I0 * f_Mn * f_Cr * f_Mo * f_Ni**—the thickest round bar reaching 50% core martensite in an infinite-severity (H = infinity) quench.

Compare Heat-Treated AISI 4140 Cr-Mo Alloy Steel Against Plain 1040 Carbon Steel at Identical 0.40% Carbon—Base_Carbon_Grain_Diameter D_I0 = 5.40 mm (B2), Manganese Mn = 0.85% (B3 -> f_Mn = 3.833 in E2), Chromium Cr = 0.95% (f_Cr = 3.052, B4), Molybdenum Mo = 0.20% (f_Mo = 1.600, B5), and Residual_Nickel Ni = 0.15% (f_Ni = 1.054, B6): Multiplicative Alloy Product reaches 19.74x (E3), boosting Ideal Critical Diameter D_I to 106.6 mm (4.20 inches in E5, vs only 18.9 mm on plain 1040 steel)!

ASTM A255 Grossmann Hardenability KPI (4140 Alloy vs Plain 1040 @ DI0=5.4 mm)FormulaVerified Output
Manganese Factor f_Mn1 + 3.333 * Mn_Pct3.833 (3.500 @ 0.75% Mn plain 1040)
Combined Alloy Multiplierf_Mn * f_Cr * f_Mo * f_Ni19.74x (3.50x @ plain 1040 carbon)
Ideal Critical Diameter DI (mm)Base_DI0_mm * Combined_Alloy_Mult106.6 mm (18.9 mm @ plain 1040)
Ideal Critical Diameter DI (in)Ideal_Critical_DI_mm / 25.44.20 in (0.74 in @ plain 1040)

ASTM A255 Multiplicative Grossmann Ideal Critical Diameter Formula

Validate Base_DI0 in (1, 15] mm, Mn in [0, 1.20]%, Cr in [0, 1.50]%, Mo in [0, 0.40]%, and Ni in [0, 1.50]% (the linear single-slope domain of ASTM A255).

=LET(dz_m, B2, mn_p, B3, cr_p, B4, mo_p, B5, ni_p, B6, fm_n, 1 + 3.333 * mn_p, fc_r, 1 + 2.16 * cr_p, fm_o, 1 + 3 * mo_p, fn_i, 1 + 0.363 * ni_p, di_m, dz_m * fm_n * fc_r * fm_o * fn_i, IF(OR(dz_m <= 1, dz_m > 15, mn_p < 0, mn_p > 1.2, cr_p < 0, cr_p > 1.5, mo_p < 0, mo_p > 0.4, ni_p < 0, ni_p > 1.5), "Invalid Alloy Range", ROUND(di_m / 25.4, 2)))

Plain AISI 1040 Carbon Steel Shallow-Hardening Check (Set Mn = 0.75%, Cr = 0, Mo = 0, Ni = 0)

Strip out the chromium and molybdenum to plain 1040 carbon steel (B3 = 0.75, B4 = 0, B5 = 0, B6 = 0): Combined Alloy Multiplier E3 collapses 5.6x from 19.74 down to 3.50, shrinking Ideal Critical Diameter D_I E4 from 106.6 mm down to 18.9 mm (0.74 in, E5)—explaining why thick 1040 axles stay soft pearlite in the core even in agitated water quench.

=IF(ISTEXT(E5), E5, ROUND(B2 * (1 + 3.333 * B3) * (1 + 2.16 * B4) * (1 + 3 * B5) * (1 + 0.363 * B6), 1))

Try the example

Use the original values or change them to test your understanding.

Further reading