Aerospace Carbon/Epoxy Prepreg Layup, Autoclave Consolidation & Laminate CPT
Autoclave Prepreg Fiber Volume & Cured Ply Thickness Formula
Calculate Zero-Void Fiber Volume Fraction Vf (%) from Resin Weight Content, Single Cured Ply Thickness CPT (mm), Total N-Ply Laminate Thickness (mm), and Cured Laminate Density (g/cm³).
Prepreg data sheets quote Resin Content by WEIGHT—converting to Fiber VOLUME Fraction shifts laminate thickness and stiffness
Aerospace prepreg rolls specify dry Fiber Areal Weight FAW (g/m², e.g. 194 gsm standard AS4 plain weave or 145 gsm UD tape) and Resin Weight Fraction W_r (e.g. 0.34 = 34 wt% epoxy), whereas micromechanics (E_1 = V_f * E_f + (1 - V_f) * E_m) and CAD mold offsets depend on Fiber Volume Fraction V_f. Because carbon fiber (rho_f ≈ 1.78 g/cm³) is 41% denser than toughened aerospace epoxy (rho_r ≈ 1.26 g/cm³), 66 wt% carbon (W_f = 1 - W_r = 0.66) occupies only V_f = (W_f / rho_f) / (W_f / rho_f + W_r / rho_r) = 57.88 vol% in a consolidated zero-void autoclave cure. Once V_f is known, Single Cured Ply Thickness follows identically from fiber mass conservation: **CPT = (FAW / (rho_f * V_f)) / 1,000** (mm).
Verify on a 16-Ply Quasi-Isotropic [0/+45/-45/90]_2s Zero-Bleed Autoclave Panel—Fiber_Areal_Weight FAW = 194.0 g/m² (B2), Net_Resin_Weight_Fraction W_r = 0.34 (34 wt%, B3), Carbon_Fiber_Density rho_f = 1.78 g/cm³ (B4), Cured_Epoxy_Density rho_r = 1.26 g/cm³ (B5 -> Fiber Volume Fraction V_f = 57.88% in E2), and Layup_Ply_Count N = 16 plies (B6): Single Cured Ply Thickness CPT equals 0.1883 mm (7.41 mils, E3), 16-Ply Laminate Thickness equals 3.013 mm (E4), and Cured Laminate Density hits 1.561 g/cm³ (E5).
| Aerospace Prepreg Autoclave KPI (FAW=194 gsm, Wr=0.34, rhof=1.78, rhor=1.26, 16 Plies) | Formula | Verified Output |
|---|---|---|
| Fiber Volume Fraction Vf (%) | ((1-Wr)/rhof) / ((1-Wr)/rhof + Wr/rhor) * 100 | 57.88% (64.54% after bleed to Wr=0.28) |
| Cured Ply Thickness CPT (mm) | (FAW_gsm / (rho_f * Vf_frac)) / 1000 | 0.1883 mm (0.1689 mm @ Wr = 0.28) |
| Total N-Ply Laminate Gauge (mm) | CPT_mm * Ply_Count_N | 3.013 mm (2.702 mm @ Wr = 0.28) |
| Cured Laminate Density (g/cm³) | Vf * rho_f + (1 - Vf) * rho_r | 1.561 g/cm³ (1.596 g/cm³ @ Wr = 0.28) |
Weight-to-Volume Prepreg Conversion & Exact Cured Ply Thickness Formula
Validate FAW > 20 g/m², Resin_Weight_Frac W_r in [0.15, 0.65], Fiber_Density > Resin_Density > 0.8 g/cm³, and integer Ply_Count N >= 1.
=LET(fa_w, B2, wr_f, B3, rf_g, B4, rr_g, B5, np_c, B6, wf_f, 1 - wr_f, vf_r, (wf_f / rf_g) / ((wf_f / rf_g) + (wr_f / rr_g)), IF(OR(fa_w <= 20, wr_f < 0.15, wr_f > 0.65, rr_g <= 0.8, rf_g <= rr_g, np_c < 1), "Invalid Prepreg Input", ROUND(vf_r * rf_g + (1 - vf_r) * rr_g, 3)))Bleeder-Cloth Resin-Bleed Consolidation Check (Set Net Cured Resin Weight Wr B3 = 0.28)
Add fiberglass bleeder plies under 6-bar autoclave pressure so excess resin bleeds down to W_r B3 = 0.28 (28 wt%): Fiber Volume Fraction E2 compacts up to 64.54%, CPT E3 thins to 0.1689 mm, 16-Ply Panel Gauge E4 drops -0.311 mm to 2.702 mm (crucial for matched-metal wing-spar clevis shimming), and Density E5 rises to 1.596 g/cm³.
=IF(ISTEXT(E5), E5, LET(wf_f, 1 - B3, vf_r, (wf_f / B4) / ((wf_f / B4) + (B3 / B5)), ROUND(((B2 / (B4 * vf_r)) / 1000) * B6, 3)))Try the example
Use the original values or change them to test your understanding.