Arte SheetsLearn. Try. Understand.

Technical & Sanitaryware Ceramics, Darcy-Washburn Plaster Slip-Casting Kinetics

Ceramic Slip Casting Parabolic Wall-Buildup Formula

Calculate Wet Cast Green Wall Thickness L = SQRT(2*K*t) (mm), Instantaneous Buildup Rate dL/dt (mm/min), Fired Ceramic Wall Thickness (mm), and Dwell Time for 8 mm Cast (min).

Doubling plaster-mold dwell time NEVER doubles ceramic cast thickness—because consolidated clay cake chokes capillary suction as SQRT(t)

During Drain Slip Casting of porcelain sanitaryware, alumina crucibles, and silicon-nitride turbine rotors, micro-porous beta-hemihydrate Plaster of Paris (CaSO_4·2H_2O) molds draw filtrate water out of deflocculated ceramic slip by ~0.1–0.2 MPa capillary suction, depositing a dense leather-hard Cast Cake of Thickness L(t) (mm) against the mold wall. Because filtrate water must percolate through the *growing* low-permeability clay/alumina cake itself (Darcy’s Law dL/dt = K / L), integrating yields **Adcock & McDowall’s Parabolic Root-Time Law L(t) = SQRT(2 * K * t) (mm), where Casting Rate Constant K (mm²/min) lumps plaster suction pressure, slip solids loading, filtrate viscosity, and cake permeability, Instantaneous Growth Rate dL/dt = K / SQRT(2 * K * t) (mm/min) decays continuously, and reaching 8.0 mm wet wall takes t8mm = 64 / (2 * K)** (4x dwell time for 2x wall thickness).

Verify on a Deflocculated Vitreous China Sanitaryware Slip—Casting_Rate_Constant K = 0.42 mm²/min (B2), Mold_Dwell_Time t = 48.0 min (B3), and Total_Wet-to-Fired_Linear_Shrinkage Stot = 11.5% (B4): Wet Green Wall L reaches 6.35 mm (E2), Instantaneous Growth Rate slows to 0.066 mm/min (E3), Post-Kiln Fired Wall equals 5.62 mm (E4), and building a heavy 8.0 mm wet rim requires 76.2 minutes before draining excess slip (E5).

Ceramic Slip-Casting KPI (t=48 min, Shrinkage=11.5%: Fresh Mold K=0.42 vs Wet Mold K=0.18)FormulaVerified Output
Wet Cast Green Wall L (mm)SQRT(2 * Casting_K_mm2_min * Dwell_min)6.35 mm (4.16 mm thin wall @ wet mold)
Instantaneous Growth Rate (mm/min)Casting_K_mm2_min / SQRT(2 * K * t)0.066 mm/min (0.043 mm/min @ K=0.18)
Fired Sintered Wall Thickness (mm)Wet_Green_Wall_mm * (1 - Shrink_Pct / 100)5.62 mm (3.68 mm slumping risk)
Dwell Time for 8.0 mm Wet Wall (min)64 / (2 * Casting_K_mm2_min)76.2 min (177.8 min = ~3 hr bottleneck)

Darcy-Washburn Parabolic Slip-Casting Cake Buildup & Fired Shrinkage Formula

Validate Casting_Rate_Constant K in [0.01, 5.0] mm²/min, Dwell_Time t in [1, 600] min, and Total_Linear_Shrinkage in [0%, 35%].

=LET(kc_r, B2, td_m, B3, sh_p, B4, IF(OR(kc_r < 0.01, kc_r > 5, td_m < 1, td_m > 600, sh_p < 0, sh_p > 35), "Invalid Slip Cast Input", ROUND(64 / (2 * kc_r), 1)))

Water-Logged / Sodium-Silicate Blinded Plaster Mold (K = 0.18 mm²/min) Thin-Cast Check (Set K B2 = 0.18)

Re-cast into a damp plaster mold saturated from the morning turn or glazed by sodium-silicate deflocculant (K drops to B2 = 0.18 mm²/min): a 48-minute timer produces only 4.16 mm wet wall (E2 -> 3.68 mm fired wall in E4, sagging during bisque firing), while reaching 8.0 mm wet wall balloons E5 to 177.8 minutes.

=IF(ISTEXT(E5), E5, ROUND(SQRT(2 * B2 * B3), 2))

Try the example

Use the original values or change them to test your understanding.

Further reading