Electroplating Surface Finishing, Watts Nickel / Hard Chrome Baths & Faraday’s Law
Faraday Electroplating Thickness & Cathode Efficiency Formula
Calculate Cathode Current Density J (A/dm²), Ideal 100%-Faradaic Deposited Mass (g), Cathode-Efficiency-Adjusted Metal Mass (g), and Mean Electroplated Coating Thickness (um).
Why hard-chrome plating builds microns 14x slower than Watts nickel at the same amperage—valence n=6 AND 82% hydrogen gas loss
By Michael Faraday’s First and Second Laws of Electrolysis (F = 96,485.33 C/mol), passing DC Rectifier Current I (A) for Immersion Time t (min -> Q = 60 * I * t coulombs) theoretically reduces m_ideal = (Q * M_mol) / (n * 96,485.33) grams of metal of Molar Mass M_mol (g/mol) and Ionic Oxidation Valence n (n = 2 for Ni^2+, Cu^2+, Zn^2+ vs n = 6 for hexavalent chromic acid Cr^6+). In real industrial plating tanks, parasitic cathode 2H+ + 2e- -> H2 hydrogen gas evolution steals 1 - eta_c of the current—leaving Cathode Current Efficiency eta_c near 92%–97% in Watts nickel or acid copper baths, yet ONLY 15%–22% in hexavalent hard-chrome tanks. Dividing Actual Metal Mass m_act = m_ideal * (eta_c / 100) by Metal Density rho (g/cm³) and Wetted Part Surface Area A_dm2 * 100 (cm²) yields Mean Coating Build delta_um = (m_act / (rho * A_cm2)) * 10,000 micrometers.
Verify on a Watts Bright-Nickel Rack Plating Bath—Rectifier_Current I = 180.0 A (B2), Immersion_Time t = 45.0 min (B3), Cathode_Efficiency eta_c = 94.0% (B4), Nickel_Molar_Mass M = 58.69 g/mol (B5), Nickel_Valence n = 2 (B6), Nickel_Density rho = 8.90 g/cm³ (B7), and Rack_Part_Area = 30.0 dm² (3,000 cm², B8 -> Current Density J = 6.00 A/dm² in E2): 100% Faradaic Mass is 147.81 g (E3), Actual Plated Nickel is 138.94 g (E4), and Mean Coating Thickness hits 52.04 um (E5).
| Faraday Electroplating KPI (180 A x 45 min on 30 dm²: Watts Ni2+ vs Cr6+ Hard Chrome) | Formula | Verified Output |
|---|---|---|
| Cathode Current Density (A/dm²) | Rectifier_Current_A / Part_Area_dm2 | 6.00 A/dm² (600 A/m²) |
| 100% Faradaic Ideal Mass (g) | (I * t_min * 60 * M_g_mol) / (n * 96485.33) | 147.81 g Ni (43.65 g @ Cr n=6) |
| Actual Deposited Metal Mass (g) | Ideal_Mass_g * (Cathode_Eff_Pct / 100) | 138.94 g Ni (7.86 g @ Cr 18% eff) |
| Mean Plated Thickness (um) | (Actual_Mass_g / (rho * Area_dm2*100))*1e4 | 52.04 um Ni (3.64 um Cr—14.3x slower) |
Faraday’s Electrolysis Law & Cathode Efficiency Micron Coating Formula
Validate Current > 0 A, Time > 0 min, Cathode_Eff in (0%, 100%], Molar_Mass > 0 g/mol, integer Valence n in [1, 8], Density > 0.5 g/cm³, and Surface_Area > 0 dm².
=LET(ia_m, B2, tm_m, B3, ef_c, B4, mm_g, B5, vn_i, B6, rh_g, B7, ar_d, B8, IF(OR(ia_m <= 0, tm_m <= 0, ef_c <= 0, ef_c > 100, mm_g <= 0, vn_i < 1, vn_i > 8, rh_g <= 0.5, ar_d <= 0), "Invalid Plating Input", LET(mi_g, (ia_m * tm_m * 60 * mm_g) / (vn_i * 96485.33), ma_g, mi_g * (ef_c / 100), ROUND((ma_g / (rh_g * ar_d * 100)) * 10000, 2))))Hexavalent Hard-Chrome Tank Comparison Check (Set Eff = 18%, M = 52.00, n = 6, rho = 7.19 g/cm³)
Run the exact same 180 A x 45 min charge in a hexavalent hard-chrome tank (B4 = 18, B5 = 52.00, B6 = 6, B7 = 7.19): 6-electron reduction cuts Ideal Mass E3 to 43.65 g, 82% hydrogen evolution slashes Actual Chromium E4 to 7.86 g, and Thickness E5 reaches only 3.64 um—explaining why hard-chrome hydraulic rods require 30–50 A/dm² and multi-hour tank cycles.
=IF(ISTEXT(E5), E5, ROUND(((B2 * B3 * 60 * B5) / (B6 * 96485.33)) * (B4 / 100), 2))Try the example
Use the original values or change them to test your understanding.