Gas Nitriding Potential KN & Case Depth Formula

Calculate Retort Ammonia Partial Pressure p_NH3 (atm), Hydrogen Partial Pressure p_H2 (atm), Lehrer Nitriding Potential KN (atm^-0.5), and Parabolic Nitrided Case Depth (mm).

Why AMS 2759/10 precision gear nitriding controls Lehrer Potential KN = p_NH3 / p_H2^(1.5) instead of archaic burette % dissociation

At 510–530 °C (below steel’s A_1 transformation so precision aerospace gears suffer near-zero quench distortion), catalytic cracking of pure 1-atm inlet ammonia (NH3 -> (1/2) N2 + (3/2) H_2) by reacted fraction alpha (0 < alpha < 1) expands 1 mole of inlet gas to 1 + alpha total exhaust moles—giving Residual Ammonia Partial Pressure pNH3 = (1 - alpha) / (1 + alpha) (atm) and **Hydrogen Partial Pressure pH2 = (1.5 * alpha) / (1 + alpha) (atm). E. Lehrer’s phase diagram proves surface iron-nitride phase formation (alpha-Fe diffusion zone vs tough gamma’-Fe_4N vs brittle spalling epsilon-Fe_2N1-x "white compound layer") is governed strictly by Thermodynamic Nitriding Potential K_N = pNH3 / (pH2^{1.5}) (atm^{-0.5}), while interstitial nitrogen diffusion drives Effective Nitriding Case Depth NHD = k_N * SQRT(thr)** (mm).

Verify on an AMS 2759/10 Two-Stage (Floe Process) 4140/4340 Gear Retort—Stage-1_Reacted_Ammonia_Fraction alpha = 0.34 (B2), Isothermal_Hold_Time t = 24.0 h (B3), and 520 °C Alloy_Diffusion_Constant k_N = 0.085 mm/h^0.5 (B4): pNH3 equals 0.4925 atm (E2), pH2 equals 0.3806 atm (E3), Nitriding Potential K_N hits 2.098 atm^-0.5 (nucleating an active nitrogen supply in Stage 1, E4), and 24-hour Case Depth reaches 0.416 mm (E5).

AMS 2759/10 Gas Nitriding KPI (1 atm NH3 Feed, t=24 h, kN=0.085, alpha=0.34 vs 0.55)FormulaVerified Output
Ammonia Partial Pressure p_NH3 (atm)(1 - alpha) / (1 + alpha)0.4925 atm (0.2903 atm @ Stage-2 0.55)
Hydrogen Partial Pressure p_H2 (atm)(1.5 * alpha) / (1 + alpha)0.3806 atm (0.5323 atm @ Stage-2 0.55)
Lehrer Nitriding Potential KN (atm^-0.5)p_NH3 / (p_H2 ^ 1.5)2.098 (0.748 white-layer suppression)
Effective Case Depth NHD (mm)Diffusion_k_mm_sqrth * SQRT(Time_hr)0.416 mm (~0.0164 in)

Stoichiometric NH3 Cracking Partial Pressures, Lehrer KN & Root-Time Depth Formula

Validate Reacted_Fraction alpha in (0.05, 0.95), Hold_Time t > 0.5 h, and Diffusion_Constant k_N in (0.02, 0.25] mm/h^0.5. Notice the common stoichiometry trap: 1 mole of NH3 reacting by fraction alpha yields 1 + alpha total moles—forgetting the (1 + alpha) denominator overestimates both pNH3 and pH2.

=LET(al_f, B2, th_r, B3, kn_d, B4, IF(OR(al_f <= 0.05, al_f >= 0.95, th_r <= 0.5, kn_d <= 0.02, kn_d > 0.25), "Invalid Nitriding Input", ROUND(kn_d * SQRT(th_r), 3)))

Floe-Process Stage-2 High Dissociation (alpha = 0.55) White-Layer Reduction Check (Set B2 = 0.55)

Raise Stage-2 ammonia cracking to alpha B2 = 0.55 (or bleed dissociated H_2/N2 gas): pNH3 E2 drops to 0.2903 atm, pH2 E3 climbs to 0.5323 atm, and Lehrer Potential K_N E4 plunges nearly 3x from 2.098 down to 0.748 atm^-0.5—dropping into the alpha-Fe / low-gamma’ region so brittle epsilon white layer dissolves inward without sacrificing 0.416 mm case depth.

=IF(ISTEXT(E5), E5, LET(pn_a, (1 - B2) / (1 + B2), ph_a, (1.5 * B2) / (1 + B2), ROUND(pn_a / (ph_a ^ 1.5), 3)))